  1. As per QW-404.37, changes in ‘’A’’ number requires re-qualification. Hence, your vendor can’t support SS 309L PQR. Need a separate PQR.(Case : 1)

 

  1. With ER309L, the final chemistry of SS 347 will not be achieved. They can support the PQR qualified with ER309L for the WPS. However, the actual WPS shall be prepared with the combination of ER309Cb+ER347 to achieve final chemistry of ER 347 as F. No is 6 for all wires.(Case :2)

 

Regards,
Vasanth


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of tong tong
Sent: 03 January 2010 13:27
To: materials-welding@googlegroups.com
Subject: [MW:3946] Overlay/cladding procedure

 

Hi ,

 

I have one query regarding above mentioned subject. Let me brief in general what actually happen in my project. My project is modification of clad column (installation of new nozzles) and associated piping. Existing cladding is SS 410S (Middle to bottom section) and SS 347 (top section). After referring to API 582 Appendix B table B-1, recommendation of filler selection for 

1. SS 410S is ER NiCr-3 for 1st and 2nd layer
2. SS 347 is ER 309Cb for 1st layer and ER 347 for 2nd layer.

I already instructed our contractor to qualified cladding procedure (GTAW process) based on ASME IX and API 582 but unfortunately our contractor refused to do it and claim their existing Cladding procedure SS 309L qualify to clad SS 410S and SS 347. 

I don't know what to do now because I'm not well known about ASME IX. Please help and advice me. You cooperation is highly appreciated

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


*** WORLEYPARSONS GROUP NOTICE *** "This email is confidential. If you are not the intended recipient, you must not disclose or use the information contained in it. If you have received this email in error, please notify us immediately by return email and delete the email and any attachments. Any personal views or opinions expressed by the writer may not necessarily reflect the views or opinions of any company in the WorleyParsons Group of Companies."

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...