Saturday, September 19, 2009

[MW:3258] Re: 3238] Shelf life of Low hydrogen electrodes

Dear

Claes Gillenius,

Please let me know how many times re drying is permissible. If electrodes are not used and kept inside the oven, but oven is turn off for overnight.

Regards,

Rafique

To: materials-welding@googlegroups.com
Subject: [MW:3240] Re: 3238] Shelf life of Low hydrogen electrodes
From: claes.gillenius@esab.se
Date: Thu, 17 Sep 2009 12:41:08 +0200


If the electrodes are packed in air tight packages they can be used right away. If not, redry the electrodes in the way the manufacturer recommends, normally at a temperature around 300 - 350 °C.
Air tight packages are for example vacuum packages. If such a package is damaged and the vacuum lost, redy the electrodes. Redrying returns the electrodes to it´s original state.

Best regards,

Claes Gillenius
Development Engineer, MMA. (Spec. stainless and non Fe-alloys)
Direct tel:  +46 (0)31 509315
Mobile +46 (0)707532012
Company                ESAB AB
Address                  Box 8004, 402 77  Gothenburg, Sweden
                                 LindholmsallĂ©n 9
Company  reg number        556005-7738



"Bathula Raghuram (Mumbai - PIPING)" <R.Bathula@ticb.com>
Sent by: materials-welding@googlegroups.com 2009-09-17 12:17
Please respond to
materials-welding@googlegroups.com


To
<materials-welding@googlegroups.com>
cc

Subject
[MW:3239] RE: 3238] Shelf life of Low hydrogen electrodes







Consult the consumable manufacturer, may be shelf life revalidated with additional testing. Code does not specify the shelf life, but the manufacturer does.



From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Ravindra T
Sent:
Thursday, September 17, 2009 3:28 PM
To:
materials-welding@googlegroups.com
Subject:
[MW:3238] Shelf life of Low hydrogen electrodes

 
Dear All
 
Our contractor has brought low hydrogen electrodes (E 7018 & 8018) which are manufactured in 2007 for welding station piping in one of our intermediate pump station of our cross country pipeline project. I would like to know whether these electrodes can be used now?. Is there any reference in ASME code regarding the expiry/ shelf life of Electrodes?
 
Please advise me in this regard.
 
Thanking you all in advance
 
Ravindra
Senior Project Engineer






This communication and any files transmitted with it contain information which is confidential and which may also be privileged. It is for the exclusive use of the intended recipient(s). If you are not the intended recipient(s), please note that any disclosure, copying, printing or use whatsoever of this communication or the information contained in it is strictly prohibited. If you have received this communication in error, please notify us by e-mail or by telephone as above and then delete the e-mail together with any copies of it. ESAB does not accept liability for the integrity of this message or for any changes, which may occur in transmission due to network, machine or software failure or manufacture or operator error. Although this communication and any files transmitted with it are believed to be free of any virus or any other defect which might affect any computer or IT system into which they are received and opened, it is the responsibility of the recipient to ensure that they are virus free and no responsibility will be accepted by ESAB for any loss or damage arising in any way from receipt or use thereof. </div



Get a 360o view of the world, in perspectives only MSN India can offer. Try it!
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...