Dear Mr.Shanmugam

Since the operating temperature is below 325 deg C , you can use E309L/ E309MoL consumable. If the operating temperature is more than 315deg C , then have to use inconel electrodes e.g. ENiCrMo-3.
 
Regards,
Amarjit Singh

On Mon, Sep 7, 2009 at 11:59 PM, Siva Shanmugam <siva196510@gmail.com> wrote:

Dear all,

I would like to know your suggestions about the filler materials for
welding of TP304H to A335 P11 for natural gas feed stock in reformer
with the working temperature around 250 deg.celcius.

Welcome for all of your valuable recommendations and suggestions.

Best regards,

R.Sivashanmugam


--
Amarjit Singh

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

Re: [MW:34913] Filler wire

E71T-1C  is Charpy Impact tested at -20degC E71T-1CJ is Charpy impact tested at -40degC. AWS Classification for FCAW is only a supplementary...