API pipe wont have P number instead it has S number.
API 5l X52 is S-1 Gr 1 material so if you have a PQR for P1 material you are automaticaly qualified for this material.
If you are doing SMAW welding then you can use E6010 for ROOT welding and E7018 for fill up and capping.
note that API 5l X 52 is equivalent to ASTM SA 106 Gr.B
hope this satisfies your requirement.
thank you
to best of my knowledge
Shammas kallinkil
QA/QC Engineer
FANOY GAS L.L.C
On Thu, Sep 10, 2009 at 4:44 AM, Juan Coello <jacoello87@gmail.com> wrote:
Hello, I'm in need of your knowledge, I need to make a WPS and a PQR
to weld two materials, both are api 5lx52 schedule 120 outside
diameter16", I cannot determine nor find the P number nor Group number
of this material.
I am also trying to determine what types of electrodes to use, wether
E60XX or E70XX if I'm not mistaken nor how many passes to make (I'm
thinking abot 6).
Thank you and hoping for a response
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---
No comments:
Post a Comment