Tuesday, September 8, 2009

[MW:3139] Re: Filler for TP304H toA335 P11

Dear Mr.Shanmugam
Since the operating temperature is below 325 deg C , you can use E309L/ E309MoL consumable, then the cost will be lower than using ENiCrMo-3 consumable. If the operating temperature is more than 315deg C , then have to use eNiCrMo-3.
 
Regards, 

On Tue, Sep 8, 2009 at 2:29 AM, Siva Shanmugam <siva196510@gmail.com> wrote:

Dear all,

I would like to know your suggestions about the filler materials for
welding of TP304H to A335 P11 for natural gas feed stock in reformer
with the working temperature around 250 deg.celcius.

Welcome for all of your valuable recommendations and suggestions.

Best regards,

R.Sivashanmugam


--
Sukamal Naskar
Malaysia



--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:34866] Presentation for WPS ,PQR AND WPQ as per ASME Sec IX in power point

Dear Experts.        If anyone having presentation of WPS,PQR and WPQ  as per ASME  SEC.IX  in power point then please share . Regards Sanja...