UTP A 80 M
AWS A 5.14 ER NiCu-7
Fe content in above mentioned filler metal =1%, Contact fabricator for Fe % after two layers, when appliing 4+ mm (+for machining) overlay.
> Subject: [MW:2919] Nicu7 Overlay
> From: amritas2001@gmail.com
> To: materials-welding@googlegroups.com
>
>
> Hi! Friends
>
> Can any one please help for to know the following
>
> i) We require to have restoration/ overlay of Monel (NiCu7)
> cladding by SMAW,TIG process ,where Specification restricts for Max
> Fe 2.5% for top 2/3 of monel (NiCu7)weld overlay (We require to weld
> overlay on SA 516Gr 70 material having thk of 10mm min). Generally
> required monel overlay thk is 4 mm.
>
> ii) Will you please guide
> a) Which is the best consumables brand to achieve Fe 2.5% max
> for top 3mm weld overlay?
> b) What is the min overlay height possible to achieve above
> requirement.?
> c) What is the best welding parameter ?
> d) Due to cost implication ,we want to achieve the required
> chemistry of NiCu7 with max 2.5% Fe at optimum overlay height of 5mm
>
> regards,
>
> AMARJIT SINGH
> TEMA INDIA LTD.,
> ACHHAD
> amarjitsingh@temaindia.com
> amritas2001@gmail.com
>
> --~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---
Comments