[MW:1964] FW: 1963] SS 410 overlay with E 309L MO barrier layer

 

 


From: Chandra, Vasanthan (Lagos) [mailto:Vasanthan.Chandra@DeltaAfrik.com]
Sent: Wednesday, April 15, 2009 8:30 PM
To: materials-welding@googlegroups.com
Subject: RE: 1963] SS 410 overlay with E 309L MO barrier layer

 

 

1. How many layers deposited with thickness of each layer including barrier layer?

2. Check for Welding consumable chemistry used for welding (Batch No wise).

3. Max Ni content for SS410 for FCAW Consumable is 0.6%. Hence, depends upon your consumable batch no, the chemistry will be achieved. We can’t get 0.6% Ni because of variation in batch no.

4. ‘’C’’ content. Again it is depends upon the batch used. Check for the same.

5. Bend failure: This is might be due to the formation of sigma phases by heat treatment. Hence, choose consumable with extra low carbon and do screening test.

 

Regards,

vasanth

 

 

 

 

 

-----Original Message-----
From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of JASPAL SINGH
Sent: 15 April 2009 07:41
To: Materials & Welding
Subject: [MW:1963] SS 410 overlay with E 309L MO barrier layer

 

 

Dear all

 

I have problem in the overlay of SS 410 on SA 516 Gr  70 with FCAW

process

 

  - I am unable to achieve the carbon % 0.06

  - failure in bend test

  - unable to achieve Ni content of 0.6%

 

As required the barrier layer of E309Lmo which contains high value of

Ni and Cr .

 

Please let me know is it possible to achieve 0.6% Ni in clad layer

with height of 6mm only.

 

how to clear the bend test ? or waiver from client is the only option.

 

Looking for you valuable suggestions.

 

JASPAL SINGH

 

919996624244

 


--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...